| ARCO Metal Specification |
(Revised
12/21/09) |
|
| For a printable PDF version of this document
click here |
 |
| Element | 3004A |
GS6 | GS7 |
3105 |
| Si | 0.22 | 0.26 | 0.30 | 0.60 |
| Fe | 0.50 | 0.60 | 0.70 | 0.70 |
| Cu | 0.26 | 0.30 | 0.35 | 0.30 |
| Mn | 0.5-1.40 | 0.3-1.6 | 0.1-2.0 | 0.3-2.0 |
| Mg | 0.7-2.0 | 0.4-2.0 | 0.1-2.4 | 0.2-2.4 |
| Pb |
0.0100 |
0.0130 |
0.0150 |
0.0150 |
| Cd | 0.010 | 0.013 | 0.015 | 0.015 |
| Zn | 0.15 | 0.18 | 0.20 | 0.35* |
| Ti | 0.02 | 0.03 | 0.04 | 0.05 |
| Na |
0.020 |
0.025 |
0.030 |
0.030 |
| Ca |
0.020 |
0.025 |
0.030 |
0.030 |
| Cr | 0.03 | 0.05 | 0.07 |
0.20* |
| B | 0.0010 | 0.0010 | 0.0010 | 0.0010 |
| Be | 0.0001 | 0.0001 | 0.0001 | 0.0001 |
| Li | 0.0005 | 0.0005 | 0.0005 | 0.0005 |
| Others Each | 0.03 | 0.04 | 0.05 | 0.05 |
| Others Total | 0.10 | 0.12 | 0.15 | 0.15 |
|
 |
| Element | 5182A |
5182B | 5182C |
| Si | 0.14 | 0.17 | 0.20 |
| Fe | 0.28 | 0.30 | 0.33 |
| Cu | 0.07 | 0.10 | 0.12 |
| Mn | 0.43 | 0.45 | 0.47 |
| Mg | 5.0-12.0 | 4.5-12.0 | 3.0-12.0 |
| Pb |
0.0100 |
0.0110 |
0.0120 |
| Cd | 0.010 | 0.013 | 0.015 |
| Zn | 0.07 | 0.10 | 0.15 |
| Ti | 0.05 | 0.06 | 0.07 |
| Na |
0.020 |
0.025 |
0.030 |
| Ca |
0.020 |
0.025 |
0.030 |
| Cr | 0.04 | 0.05 | 0.06 |
| B | 0.0010 | 0.0010 | 0.0010 |
| Be | 0.0001 | 0.0001 | 0.0001 |
| Li | 0.0005 | 0.0005 | 0.0005 |
| Others Each | 0.03 | 0.04 | 0.05 |
| Others Total | 0.10 | 0.12 | 0.15 |
|
 |
The above are maximums expressed in percent of total
Others each includes: Bi, Ni, Sn, Zr, V
Others total includes: Ti, Na, Ca, Cd, Pb, Be, Ni, Cr, Sn, V, Zr, B.
Must be low profile sow or standard T-Bar
All pieces must be marked with heat number
*Preferred Cr<.15, Zn<.30 |
 |
| Element Reporting Requirements for
RSI and primary aluminum are shown below. |
Lithium
Material from reduction plants using Lithium in their process is not acceptable.
RSI Sow Heat Variation
Maximum heat variation for all ARCO Specs must be no greater than 150% of the
average per element. Heat variation greater than 150% of the average per element
will not be accepted without prior approval from ARCO.
Italicized numbers in the
specification tables above are
absolute maximums by heat,
unless otherwise approved in
advance of shipment.
Loading of RSI Sow
Please load heats on truck/railcar in the same order as listed on the COA sheet.
This does not apply to prime aluminum.
For additional shipping requirements
click here
for the RSI/Prime/Meltable Shipping and Receiving page.
Prime Standards
Aluminum Association Gold Sheets
- International Designations and
Chemical Composition Limits for
Unalloyed Aluminum - North American
and International Registration
Record, March, 2007 can be obtained
from:
http://www.aluminum.org
Element Reporting Requirements
|
| Name | Symbol |
RSI (40) | Prime Aluminum
(30) | Slab, Plate, Coil, Other * (16) |
Decimal Reporting |
| Silicon | Si | Y | Y | Y | 3 |
| Iron | Fe | Y | Y | Y | 3 |
| Copper | Cu | Y | Y | Y | 3 |
| Manganese | Mn | Y | Y | Y | 3 |
| Magnesium | Mg | Y | Y | Y | 3 |
| Chromium | Cr | Y | Y | Y | 3 |
| Nickel | Ni | Y | | Y | 3 |
| Zinc | Zn | Y | Y | Y | 3 |
| Titanium | Ti | Y |
Y | Y | 3 |
| Boron | B | Y | Y | Y | 4 |
| Sodium | Na | Y | Y | Y | 4 |
| Calcium | Ca | Y | Y | Y | 4 |
| Lithium | Li | Y | Y | Y | 4 |
| Vanadium | V | Y | Y | Y | 4 |
| Lead | Pb | Y |
R** | Y | 4 |
| Tin | Sn | Y | | Y | 4 |
| Bismuth | Bi | Y | | Y | 4 |
| Beryllium | Be | Y | | Y | 4 |
| Cadmium | Cd | Y | | Y | 4 |
| Phosphorus | P | Y | | Y | 4 |
| Antimony | Sb | R** | | Y | 4 |
| Zirconium | Zr | Y | | | 4 |
| Gallium | Ga | Y | Y | Y | 4 |
| | | | | |
|
* Aluminum alloys, excludes prime aluminum and RSI ** R=Recommended |